Acid wash

Ultimate affect of Acid wash

•During Acid wash, pumic stones are used. By the action of pumic stones, irregular faddeng affect is developed on the heavy garments like denims, thick canvas/twill, and sweater. The pumic stones act a brushing action on the garment fabric surface. The area where more brushing action takes place there more dicolour or fadding affect is developed and the area where less brushing action takes place less brushing action and takes place less fadding affect will be developed. The multi-layer fabric areas like –collar, calf, pocket, placket, side seam etc area will be brushed more than the single layer areas. As a result irregular fadding affect will be developed on the garments fabric surface. Thus in this way fadding affect may be developed on the garment by acid wash technique.

ACID WASH PROCESS

A processor Acid wash of 60 kg batch of Denim Trouser as mentioned below:-

First Step: -Pretreatment/Desizing.

•Add water @ L : R = 1 : 10 .............. 600 litres.

•Start Machine.

•Add desizing agent @ 1 gm/litre .................600 Gms.

•Add detergent @ 1 gm/litre ........................ 600 Gms.

•Temperature............................. 60°c.

•Time........................... 20 mts.

•Drop the liquor.

•Rinse one for 3 minutes (cold).

Second Step:-Hot wash

•Add water @ L: R = 1: 10.............. 600 litres.

•Temperature............................. 60°c.

•Time........................... 5 mts.

•Drop the liquor.

•Here hot wash is used to remove the adhering materials from the garment surface.

•Unload the garments from the washing m/c in the trolley.

•Load the pre treated garments in the dryer m/c.

•Dry the garment completely & unload the garments.

•The pumic stones used for acid wash need to pre-treat in the following chemical solution:-

•Water ..................... 100 L

•Potassium per manganate.............. 1000 Gms.

•Phosphoric Acid............................... 250 Gms.

•Stire the solution in a stainless steel tub with dry pumic stone.

•Soak the stones with the chemical solution ......... 10 –15 minutes.

•The stones will pick up the solution. Then the soaked stones are dried in the open air for.............. 2 to 3 hrs.

•Then pre-treated garment 30 –40 kg per batch load in the dry washing machine.

•Load the per-treated stones (about 50 kg) in washing machine.

•Start machine running for each batch ........................ 7 to 10 mts.

•Stop machine running.

•Unload the treated garment separately. Pumic stones with P.P. solution hit on garment surface as a result fadding will be developed.

•Then load the stones treated garment in another washing machine.

•Third Step:-Wash for cleaning

•Batch wt................................ 70 kg.

•Add water @ L: R = 1: 8.............. 560 litres.

•Add detergent @ 1 gm/litre .............560 Gms.

•Temperature............................. 40°c -50°c.

•Time ..................................10 mts.

•Drop the liquor.

•Here detergent is used to remove the breaking stone dust and chemicals from the garment surface.

•Fourth Step:-Whitening/Neutralization.

•Add water @ L: R = 1: 8.............. 560 litres.

•Machine running.

•Add Metabisulphite @ 5 gm/litre..... 2800 Gms.

•Cold temperature.

•Time 5 mts.

•Drop the liquor.

•Fifth Step:-

•Add water @ L: R = 1: 7.............. 490 litres.

•Machine running.

•Add Acetic acid @ 0.6 gm/litre ..................... 294 Gms.

•Add Softner @ 1 gm/litre ........................ 490 Gms.

•Then unload the garments.

•Sixth Step:-Hydro extractor machine.

•Hydro extractor machine to remove excess water from the garments.

•Seventh Step:-Dryer machine.

•After hydro extraction the garments are sent to drying m/c for complete drying.

•Eighth Step:-Quality & Delivery.

•After drying the garments go to quality checking & rectify washing fault and then good one delivery.

Precaution:-

•Maintain the stock solution properly constant when comes socking the stone.

•No water licks age in to the machine when treated pumic stone & garments in to the machine.

•Not excess load the garments in the Acid wash processing.

•Add some new stone after finishing on batch to maintain the volume for 2nd batch. It is a mater of experience.

Colour Shade Variation & Solution

•When fabrics come in to garment factory against any order from abroad / local fabric dyeing factory, its found different colour shade roll in the same colour i.e. slide light, slide dark, slide tone different for this reason garment factory to control shade variation works as follows :-

•8"×8" size fabric cut from every roll.

•Marking roll number by permanent marking pen at back side of cutpes.

•Every cutpes joint each other and make a blanket.

•Then it washes into standard approval shade.

•Garment factory now segregate same colour tone in one bundle and shade grading A.B.C.D.

•First A shade roll cutting by pattern then B.C.D shade separately.

•After garment making shade level attached on body.

•Then go to washing plant for standard washing.

•Washing plant shade level wise washing in respective wash.

•After wash it any big shade variation found then again rewash to match with buyer approval standard.

•Final quality checking garment go to finishing section for thread cutting, button attached, iron & poley etc.

•Sand Blasting

→Popular dry process.

→A mechanical process.

→Aluminum oxide (Al203) used which looks like SAND.

→Sand blasting is performed with combine the wash like normal Wash, Stone-enzyme, Enzyme, Bleach wash etc

•Washing Process on Denim/Canvas/Twill garments

→Al2o3is very fine & very hard/Sharp.

→ Aluminum oxides (Al203) through by GUN with dry air to perform blasting action.

→The Gun has a switch to start & stop the flow.

→The garments to be sand blasting are placed on the bed of a close chamber.

→Garments are faded by frictional affect of Al2o3.

→Al2o3 flow is done at 10Ó©-20Ó©angles.

→Operators should have protective masks, gloves, Helmet, earflap, uniform.

→After mechanical fading, chemicals treatment are required.

Whisker:

•To make whisker first, Buyer’s given design is plotted on a tracing paper. Then from the tracing paper the design is transferred to the ply-wood or gas kit.

•The next step is to place foam rubber according to the design on ply wood with the help of solution gum.

•Finally, the upper surface of the rubber is grinded to a slope or spherical shape and the whisker pattern is prepared.

•Now this pattern is entered through the front opening of the pant and rubbing is done by emery paper at 320 ppm to 500 ppm. Thus the effect produced on the pant is called whisker.

•It may require more or less than 3 efforts to make whisker pattern to make buyer’s design accurately.

Hand scrapping:

•To create the impression or visibility of pocketing fabric or any inside materials visibility to the face of the jeans pants with the help of emery paper scrapping is called hand scraping. It is used as the alternatives of sand blasting in some cases.

PP Spray( Potasium per manganate spray):

•PP Spray (KMnO4: Potassium per Manganate Spray):

•10 g KMnO4 in 1 litre

•0r+ Lubricant 1%

•5 g KMnO4 in 1 litre

•For pp spray, the garments are placed in a cabinet. Then KMnO4 solution is sprayed according to the requirement.

•After spraying the garments look grayish brown.

•Then it is neutralized with oxalic acid (COOH-COOH). Finally, faded (white) effect is produced.

•Caution:

•-The worker must put on mask and hand gloves.

•-There must have back glass fountain system to avoid spreading of KMnO4 in air.

•-It is never done on grey garments. The garments must be desized before spraying.

Nano finish:

Nano process of applying resin and fluro-carbons. It is also a permanent chemical process. Following are the nano finish advantages:

•1.Water, oil and alcohol repellency but air permeability.

•2. The crease resistance feature keep clothing neat.

•3. Dye fastness can be improved and wet increases.

•4. It also helps to improve resilience, handle and drapping properties of the fabric.

•Recipe:

•Wetting agent: 0.5-1 % on the wt of the goods.

•Resin: 4-6 % owf

•Softener: 2-3 % owf (non ionic)

•Fluoro carbon: 4-6 %

Wrinkle free:

•This process is one kind of resin finishing process. In this process of applying resins on the textile material that they cross linked with the amorphous block the free (-OH) that prevent the hydrogen bond formation and thus improve the wrinkle free finishing.

•Mainly it is applied on twill fabrics, single jersey, and Denim fabric.

Some advantages:

•Improve resistance and recovery to creasing by wrinkle free process.

•Good water repellency and moderately soil repellency and remove of soil by washing can be achieved by wrinkle free process.

•Resin improves resilience, handle and draping properties of fabric.

•Improve wet and dye fastness.

Recipe:

•Wetting agent: 0.5 % on the weight of the fabric.

•resin: 6-10 % ,,

•Softener: 3-5 % ,,

•Then make 60-80 liter liquor put in the machine tank.

Product package:

•It is also known as Technical package and Merchandisers Detailed sheet.

•It contains:

•Style number of the garments.

•Item description of the garments.

•Design/Specifications of the garments.

•Measurement list of the garment.

•Color of the garments.

•Color combination of the garments.

•Size of the garments.

•Packing Instruction of the garments.

•Folding instruction of the garment.

•Types of sewing thread used.

•Instruction for care label.

•Types of the fabric used and weight of that fabric.

•Composition and contribution of that fabric.

Some Buyers condition about the Ph:

•American Eagle: 6.8-8.0

•V.F.A: 5.5-8.0

•LEVIS: 5.0-9.0

•SEARS: 6.0-8.0

•J.C.P: 5.0-9.0

•H&M: 4.5-7.5

•AMC: 6.0-8.0

•GAP: 6.0-8.0

Post a Comment

0 Comments